Abstracts
This study investigated the effect of the incorporation of an iodonium salt in experimental composites, on the bond strength of metallic brackets bonded to bovine teeth. Two hundred and seventy bovine teeth were embedded in self-curing acrylic resin and divided into 18 groups (n=15), according to the experimental composite with an iodonium salt at molar concentrations 0 (control), 0.5, or 1%; the light-activation times (8, 20 and 40 s); and the storage times (10 min or 24 h). Metallic brackets were fixed on the tooth surface using experimental composites. Photoactivation was performed with a quartz-tungsten-halogen light-curing unit curing unit for 8, 20 and 40 s. The specimens were stored in distilled water at 37 °C for 10 min or 24 h and submitted to bond strength test at 0.5 mm/min. The data were subjected to three-way ANOVA and Tukey's test (α=0.05). The Adhesive Remnant Index (ARI) was used to classify the failure modes. The shear bond strengths (MPa) at 10 min for light-activation times of 8, 20 and 40 s were: G1 - 4.6, 6.9 and 7.1; G2 - 8.1, 9.2 and 9.9; G3 - 9.1, 10.4 and 10.7; and at 24 h were: G1 - 10.9, 11.1 and 11.7; G2 - 11.8, 12.7 and 14.2; G3 - 12.1, 14.4 and 15.8. There was a predominance of ARI score 3 for groups with 10 min storage time, and ARI score 2 for groups with 24 h storage time. In conclusion, the addition of iodonium salt (C05 and C1) to the experimental composite may increase the bond strength of brackets to bovine enamel using reduced light exposure times
shear bond strength; aging; bonding; Orthodontics; polymerization; composite
Estudo investigou o efeito da incorporação de um sal de iodônio em compósito experimental, na resistência de união de braquetes metálicos fixados em dentes bovinos. Duzentos e setenta dentes bovinos foram embutidos e divididos em 18 grupos (n=15), de acordo com o compósito experimental com sal de iodônio na concentração molar de 0 (controle), 0,5 e 1 %; tempo de fotoativação (8, 20 e 40 s); e, tempo de armazenagem (10 min e 24 h). Braquetes metálicos foram fixados na superfície do dente usando compósitos experimentais. A fotoativação foi efetuada com o aparelho XL 2500 por 8, 20 e 40 s. As amostras foram armazenadas em água destilada a 37º C por 10 min e 24 h e submetidos ao ensaio de resistência de união à velocidade de 0,5 mm/min. Os dados foram submetidos à Análise de variância de 3 fatores e ao teste de Tukey (α=0,05). O Índice de Remanescente do Adesivo (IRA) foi usado para classificar os modos de falhas. Os valores de resistência de união ao cisalhamento (MPa) no período de 10 min para os tempos de fotoativação de 8, 20 e 40 s foram: G1 - 4,6; 6,9 e 7,1; G2 - 8,1; 9,2 e 9,9; G3 - 9,1; 10,4 e 10,7; e no período de 24 h foram: G1 - 10,9; 11,1 e 11,7; G2 - 11,8; 12,7 e 14,2; G3 - 12,1; 14,4 e 15,8. Houve predominância de escore 3 para os grupos armazenados por 10 min e escore 2 para os grupos armazenados por 24 h. Em conclusão, a adição do sal de iondônio (C05 e C1) em compósitos experimentais pode aumentar a resistência de união de braquetes ao esmalte bovino usando reduzidos tempos de fotoativação
Introduction
Metallic brackets are routinely bonded to the teeth using light-cured composite
resins (11 Romano FL, Correr AB, Correr-Sobrinho L, Magnani MB, Ruellas AC.
Clinical evaluation of the failure rates of metallic brackets. J Appl Oral Sci
2012;20:228-234.
2 Costa AR, Correr AB, Puppin-Rontani RM, Vedovello SA, Valdrighi HC,
Correr-Sobrinho L, et al.. Effects of thermocycling and light source on the bond
strength of metallic brackets to bovine teeth. Braz Dent J
2011;22:486-489.-33 Correr AB, Costa AR, Lucato AS, Vedovello SA, Valdrighi HC,
Vedovello Filho M,. Correr-Sobrinho L Effect of activation mode on shear bond
strength of metallic brackets. Braz Dent J 2013;24:513-516.). The advantage of photoactivated composites is that the clinician has
the control of working time to place the brackets in the correct position, easy
removal of the excess composite and possibility of immediate insertion of the
orthodontic archwire (44 Sfondrini MF, Cacciafesta V, Scribante A, Klersy C. Plasma arc
versus halogen light curing of orthodontic brackets: a 12-month clinical study
of bond failures. Am J Orthod Dentofacial Orthop
2004;125:342-347.). Adequate early
polymerization is necessary for brackets bond to the teeth resist the placement of
the orthodontic archwire. However, complete polymerization of the composite may not
be always possible when considering the clinically used light exposure times (55 Staudt CB, Krejci I, Mavropoulos A. Bracket bond strength dependence
on light power density. J Dent 2006;34:498-502.).
Composite material requires adequate light irradiance and wavelength (400-500 nm) to activate the photosensitizer camphorquinone (CQ), which reacts with an amine co-initiator to generate free radicals for polymerization (66 Rueggeberg F. Contemporary issues in photocuring. Compend Contin Educ Dent Suppl. 1999;25:4-15.,77 Stansbury JW. Curing dental resins and composites by photopolymerization. J Esthetic Dent 2000;12:300-308.). According to the manufacturers' instructions, light exposure times between 20 and 40 s are required to bond brackets to the teeth to obtain high bond strength (88 Sfondrini MF, Cacciafesta V, Pistorio A, Sfondrini G. Effects of conventional and high-intensity light-curing on enamel shear bond strength of composite resin and resin-modified glass-ionomer. Am J Orthod Dentofacial Orthop 2001;119:30-35.). However, long exposure times are uncomfortable for the patient and present drawbacks for the clinician (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.).
Some methods to reduce the light-curing time for bonding orthodontic brackets are
proposed in the literature (22 Costa AR, Correr AB, Puppin-Rontani RM, Vedovello SA, Valdrighi HC,
Correr-Sobrinho L, et al.. Effects of thermocycling and light source on the bond
strength of metallic brackets to bovine teeth. Braz Dent J
2011;22:486-489.,99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS,
Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel
using experimental composites with an iodonium salt. Eur J Orthod
2014;36:297-302.
10 Oesterle LJ, Newman SM, Shellhart WC. Rapid curing of bonding
composite with a xenon plasma arc light. Am J Orthod Dentofacial Orthop
2001;119:610-616.
11 Staudt CB, Mavropoulos A, Bouillaguet S, Kiliaridis S,. Krejci I
Light-curing time reduction with a new high-power halogen lamp. Am J Orthod
Dentofacial Orthop 2005;128:749-754.-1212 Gonçalves PR, Moraes RR, Costa AR, Correr AB, Nouer PR, Sinhoreti
MA, et al.. Effect of etching time and light source on the bond strength of
metallic brackets to ceramic. Braz Dent J 2011;22:245-248.).
The main method proposed is using light-curing units with high irradiance (e.g.
xenon plasma arc and lasers) for fast polymerization (1313 Talbot TQ, Blankenau RJ, Zobitz ME, Weaver AL, Lohse CM, Rebellato
J. Effect of argon laser irradiation on shear bond strength of orthodontic
brackets: an in vitro study. Am J Orthod Dentofacial Orthop
2000;118:274-279.,1414 Klocke A, Korbmacher HM, Huck LG, Kahl-Nieke B. Plasma arc curing
lights for orthodontic bonding. Am J Orthod Dentofacial Orthop
2002;122:643-648.), but these units
are expensive. Another alternative is the use of an iodonium salt. It has been
reported that the use of iodonium salt has shown satisfactory results for dental
adhesives when used associated with CQ (1515 Ogliari FA, Ely C, Petzhold CL, Demarco FF, Piva E. Onium salt
improves the polymerization kinetics in an experimental dental adhesive resin. J
Dent 2007;35:583-587.).
The theory that explains the performance of iodonium salts is that the CQ, after
excited by the curing light, can promote decomposition of the iodonium salt and
enhance the polymerization kinetics (1515 Ogliari FA, Ely C, Petzhold CL, Demarco FF, Piva E. Onium salt
improves the polymerization kinetics in an experimental dental adhesive resin. J
Dent 2007;35:583-587.,1616 Odian G. Introduction. In: Principles of Polymerization, 4th
Edition. John Wiley & Sons, Inc.: Hoboken, USA; 2004.).
Bond strength tests are usually carried out 24 h after the orthodontic brackets are bonded to the teeth. However, this is not what occurs in the clinical practice, where the insertion of the orthodontic archwire occurs minutes after the brackets are bonded. Several studies have shown that 24 h after the bonding procedure, the brackets bond strength increased in relation to the times of 5, 10, and 30 min (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.,1717 Bishara SE, Von Wald L, Olsen ME, Laffoon JF. Effect of time on the shear bond strength of glass ionomer and composite orthodontic adhesives. Am J Orthod Dentofacial Orthop 1999;116:616-620.,1818 Oliveira AS, Barwaldt CK, Bublitz LS,. Moraes RR Impact of bracket displacement or rotation during bonding and time of removal of excess adhesive on the bracket-enamel bond strength. J Orthod 2014;41:124-127.). There is no consensus as regards the waiting time required before placing the brackets.
The aim of this study was to investigate the effect of the incorporation of a iodonium salt in experimental composites on the shear bond strength of metallic orthodontic brackets bonded to bovine teeth, using different storage times (10 min or 24 h). The hypotheses tested were that 1) the incorporation of an iodonium salt in experimental composites would lead to higher shear bond strengths, 2) the storage time (10 min or 24 h) would not affect the shear bond strengths, and 3) specimens light-activated for longer periods would have higher shear bond strengths.
Material and Methods
Experimental Composites
This study is a follow up of the investigations on the use of iodonium salts to improve the polymerization of resin-based dental cements (9,19). The three experimental materials tested were obtained using diphenyliodonium hexafluorphosphate (DPIHFP; Sigma-Aldrich, Milwaukee, WI, USA) at molar concentrations of 0 (control), 0.5, or 1%. A model dimethacrylate co-monomer was obtained by mixing the monomers bisphenol-A glycidyl dimethacrylate (Esstech, Essington, PA, USA) and triethylene glycol dimethacrylate (Esstech) at a 70:30 mass ratio. The photoinitiating system consisted of ethyl-4 dimethylamino benzoate (EDAB; Sigma-Aldrich) and CQ (Esstech), each added at a molar concentration of 1%. Butylated hydroxytoluene (0.1 mol%) was added as radical scavenger. The blends were loaded with a 60 mass% of silanized strontium-based glass particles with 1 µm average particle size to control composite viscosity and render it thixotropicity.
Bonding Procedures
Two hundred and seventy bovine mandibular incisors without cracks were collected. The teeth were embedded in self-curing acrylic resin (Clássico Produtos Odontológicos Ltda., São Paulo, SP, Brazil) using polyvinyl chloride tubes as molds, leaving the buccal face perpendicular to the horizontal axis. The buccal faces of all teeth were cleaned using a rubber cups with non-fluoridated pumice-water slurry for 10 s, rinsed with air-water spray for 10 s and air-dried for 10 s. The teeth were divided into 18 groups (n=15), according to three experimental bonding materials (control, C05 and C1); light-activation time (8, 20 and 40 s) and storage time (10 min or 24 h). The middle third of the buccal vestibular face of all teeth was etched with 37% phosphoric acid gel (3M ESPE, St. Paul, MN, USA) for 30 s, rinsed with air-water spray for 30 s and air dried for 30 s. One layer of Single Bond 2 Adhesive (3M ESPE) was applied on the teeth, gently dried for 5 s, and photoactivated for 10 s with a quartz-tungsten-halogen light-curing unit (XL2500; 3M ESPE) with 800 mW/cm2 irradiance.
Stainless steel standard maxillary central incisor brackets (slot 0.022"; Ortodontia Morelli, Sorocaba, SP, Brazil) were positioned and seated firmly on the tooth surface. Excess bonding material was removed using a microbrush (KG Sorensen, Cotia, SP, Brazil) and light-activation was carried out with one exposure on each of the four sides of the bracket, with total exposure times of 8, 20, or 40 s. The specimens were stored in distilled water at 37 °C for 10 min or 24 h.
Bond Strength Testing and Failure Analysis
The shear bond strength (SBS) test was conducted in a mechanical testing machine (Model 4411; Instron, Canton, MA, USA) using a knife-edged rod at a crosshead speed of 1.0 mm/min until failure. A mounting jig was used to align the tooth-bracket interface parallel to the testing device. The SBS values were calculated in MPa and analyzed using three-way ANOVA and Tukey's test (α=0.05). After debonding, tooth and bracket surfaces were examined with a stereomicroscope (Olympus Corp, Tokyo, Japan) under 8× magnification. The Adhesive Remnant Index (ARI) (2020 Artun J, Bergland S. Clinical trials with crystal growth conditioning as an alternative to acid-etch enamel pretreatment. Am J Orthod 1984;85:333-340.) was used to classify the failure modes, according to: score 0 indicates that no bonding resin remained on the tooth; score 1 indicates that less than half of the bonding resin remained on the tooth; score 2 indicates that more than half of the bonding resin remained on the tooth; and score 3 indicates that all bonding resin remained on the tooth, along with a clear impression of the bracket mesh.
Results
The results for shear bond strength of brackets to teeth are shown in Table 1. For 10 min storage time, the control group showed significantly lower (p<0.05) shear bond strengths than the other bonding materials for all light-activation times. After 24 h storage, the experimental composite C1 had significantly higher (p<0.05) SBS than the control composite when light-activated for 20 and 40 s. No statistically significant differences (p>0.05) were detected when light-activated for 8 s. In the comparison of C05 and C1, no significant differences (p<0.05) were observed for storage time or light-activation time.
When the light-activation times were compared at 10 min storage time, the control group light-activated for 8 s showed significantly lower shear bond strength (p<0.05) than groups light-activated for 20 and 40 s, except for the groups C05 and C1 (p<0.05). At 24 h, the C1 experimental composite light-activated for 40 s had significantly higher SBS (p<0.05) than the group light-activated for 8 s. No significant difference was detected for control group and C05 (p>0.05). The SBS for 24 h storage time was significantly higher (p<0.05) when compared to 10 min for all groups (bonding material or light-activation time). The results for ARI are shown in Figure 1. There was a predominance of score 3 was observed for groups stored for 10 min, and score 2 was the most frequent for groups stored for 24 h.
Frequency distributions (%) of the Adhesive Remnant Index (ARI) scores for all groups. Score 0 indicates that no bonding resin remained on the tooth; Score 1 indicates that less than half of the bonding resin remained on the tooth; Score 2 indicates that more than half of the bonding resin remained on the tooth; and Score 3 indicates that all bonding resin remained on the tooth, along with a clear impression of the bracket mesh.
Discussion
The first hypothesis tested was accepted. Generally, an increased SBS was observed when DPIHFP-modified agents were incorporated in experimental composites for all light-activation times. This finding is in agreement with a previous study with experimental composites, which also found significantly higher SBS in relation to the control group, but using diphenyliodonium chloride (DPC) as iodonium salt (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.). The higher bond strength of experimental composites using DPIHFP-modified agents may be explained by the fact that the salt, even in low concentration, can promote higher polymerization reactivity. According to Ogliari et al. (1515 Ogliari FA, Ely C, Petzhold CL, Demarco FF, Piva E. Onium salt improves the polymerization kinetics in an experimental dental adhesive resin. J Dent 2007;35:583-587.) the introduction of DPIHFP as co-initiator showed significant effect on the monomer conversion. In the ternary photo-initiator system, formed by CQ, EDAB and DPIHFP, the DPIHFP may react with inactive CQ radicals formed during polymerization to decrease the termination rate and improve the initiation rate by producing new radicals from the salt fragmentation, improving the monomer reactivity in relation to two-component initiator systems (1616 Odian G. Introduction. In: Principles of Polymerization, 4th Edition. John Wiley & Sons, Inc.: Hoboken, USA; 2004.,2121 Kim D,. Stansbury JW Kinetic pathway investigations of three component photoinitiator systems for visible-light activated free radical polymerizations. J Polymer Science Part A: Polymer Chemistry 2009;47:887-898.,2222 Padon KS, Scranton AB. A mechanistic investigation of a three component radical photoinitiator system comprising methylene blue, N-methyldiethanolamine, and diphenyliodonium chloride. Journal of Polymer Science Part A: Polymer Chemistry 2000;38:2057-2066.). An increase of the polymerization rate is advantageous to the development of experimental composites by reducing curing time. When the two concentrations of DPIHFP were compared, no statistically significant difference in shear bond strength was found for all light-activation times. In this study, increased molar concentration of iodonium salt did not increase the curing reactivity of the experimental composite. These results agree with those of a previous study where lower concentrations of iodonium salt had minor influence on the polymerization rate (1515 Ogliari FA, Ely C, Petzhold CL, Demarco FF, Piva E. Onium salt improves the polymerization kinetics in an experimental dental adhesive resin. J Dent 2007;35:583-587.).
The second hypothesis was rejected, since significant differences were observed between shear bond strength for storage time at 24 h in relation to 10 min for all groups (bonding material or light-activation time). This result is in agreement with other studies, where the shear bond strength increased after 24 h in relation to 10 min (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.,1717 Bishara SE, Von Wald L, Olsen ME, Laffoon JF. Effect of time on the shear bond strength of glass ionomer and composite orthodontic adhesives. Am J Orthod Dentofacial Orthop 1999;116:616-620.,1818 Oliveira AS, Barwaldt CK, Bublitz LS,. Moraes RR Impact of bracket displacement or rotation during bonding and time of removal of excess adhesive on the bracket-enamel bond strength. J Orthod 2014;41:124-127.). According to Leung et al. (2323 Leung RL, Fan PL, Johnston WM. Post-irradiation polymerization of visible light-activated composite resin. J DentRes 1983;62:363-365.), post-polymerization of the composite, mainly in the first 24 h, may be responsible for increase in SBS. For other authors (2424 Burtscher P. Stability of radicals in cured composite materials. Dent Mater1993;9:218-221.,2525 Mohamad D, Young RJ, Mann AB, Watts DC. Postpolymerization of dental resin composite evaluated with nanoindentation and micro-Raman spectroscopy. Arch Orofacial Scienc 2007;2:26-31.), any alteration in conversion in the latter curing stages may increase polymer crosslinking and improve polymer properties.
When light-activation times were compared, the SBS of the groups light-activated for 20 and 40 s at 10 min was significantly higher than for 8 s of the control group. No statistically significant differences were found among the light-activation times for the other groups tested at 10 min or groups tested at 24 h. Therefore, the third hypothesis was partly accepted. According to Rueggeberg (55 Staudt CB, Krejci I, Mavropoulos A. Bracket bond strength dependence on light power density. J Dent 2006;34:498-502.), polymerization of resin materials is dependent on the radiant exposure, which is the product of irradiance and exposure time. In this study, approximately 6.4, 16 and 32 J/cm2 energy doses were used for specimens light-activated for 8, 20 and 40 s. These differences in energy doses may explain the difference among the light-activation times for the control group at 10 min storage time.
The results of ARI scores indicated that the majority of debonding failures left all bonding resin on the tooth, along with a clear impression of the bracket mesh (score 3) at 10 min storage time and prevalence of score 2, where more than half of the bonding resin remained on the tooth, at 24 h storage time. Similar results were found in a previous study using iodonium salt-modified agents (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.). According to Costa et al. (99 Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.), failures of modified materials tended to include fracture of the bonding material, indicating a better mechanical interlocking of the experimental composite with the bracket mesh, probably by improvements in the polymerization due to the addition of iodonium salt. In conclusion, the present study demonstrated that the addition of iodonium salt in the experimental composites may increase the bond strength of brackets bonded to bovine enamel using reduced light exposure times.
Acknowledgements
This study was supported by the Conselho Nacional de Desenvolvimento Científico e Tecnológico - CNPq (Grant #303928/2009-3). The authors acknowledge Esstech Inc. for supplying the reagents used in this study
References
-
1Romano FL, Correr AB, Correr-Sobrinho L, Magnani MB, Ruellas AC. Clinical evaluation of the failure rates of metallic brackets. J Appl Oral Sci 2012;20:228-234.
-
2Costa AR, Correr AB, Puppin-Rontani RM, Vedovello SA, Valdrighi HC, Correr-Sobrinho L, et al.. Effects of thermocycling and light source on the bond strength of metallic brackets to bovine teeth. Braz Dent J 2011;22:486-489.
-
3Correr AB, Costa AR, Lucato AS, Vedovello SA, Valdrighi HC, Vedovello Filho M,. Correr-Sobrinho L Effect of activation mode on shear bond strength of metallic brackets. Braz Dent J 2013;24:513-516.
-
4Sfondrini MF, Cacciafesta V, Scribante A, Klersy C. Plasma arc versus halogen light curing of orthodontic brackets: a 12-month clinical study of bond failures. Am J Orthod Dentofacial Orthop 2004;125:342-347.
-
5Staudt CB, Krejci I, Mavropoulos A. Bracket bond strength dependence on light power density. J Dent 2006;34:498-502.
-
6Rueggeberg F. Contemporary issues in photocuring. Compend Contin Educ Dent Suppl. 1999;25:4-15.
-
7Stansbury JW. Curing dental resins and composites by photopolymerization. J Esthetic Dent 2000;12:300-308.
-
8Sfondrini MF, Cacciafesta V, Pistorio A, Sfondrini G. Effects of conventional and high-intensity light-curing on enamel shear bond strength of composite resin and resin-modified glass-ionomer. Am J Orthod Dentofacial Orthop 2001;119:30-35.
-
9Costa AR, Vedovello-Filho M, Correr AB, Vedovello SAS, Puppin-Rontani RM, Ogliari FA, et al.. Bonding orthodontics brackets to enamel using experimental composites with an iodonium salt. Eur J Orthod 2014;36:297-302.
-
10Oesterle LJ, Newman SM, Shellhart WC. Rapid curing of bonding composite with a xenon plasma arc light. Am J Orthod Dentofacial Orthop 2001;119:610-616.
-
11Staudt CB, Mavropoulos A, Bouillaguet S, Kiliaridis S,. Krejci I Light-curing time reduction with a new high-power halogen lamp. Am J Orthod Dentofacial Orthop 2005;128:749-754.
-
12Gonçalves PR, Moraes RR, Costa AR, Correr AB, Nouer PR, Sinhoreti MA, et al.. Effect of etching time and light source on the bond strength of metallic brackets to ceramic. Braz Dent J 2011;22:245-248.
-
13Talbot TQ, Blankenau RJ, Zobitz ME, Weaver AL, Lohse CM, Rebellato J. Effect of argon laser irradiation on shear bond strength of orthodontic brackets: an in vitro study. Am J Orthod Dentofacial Orthop 2000;118:274-279.
-
14Klocke A, Korbmacher HM, Huck LG, Kahl-Nieke B. Plasma arc curing lights for orthodontic bonding. Am J Orthod Dentofacial Orthop 2002;122:643-648.
-
15Ogliari FA, Ely C, Petzhold CL, Demarco FF, Piva E. Onium salt improves the polymerization kinetics in an experimental dental adhesive resin. J Dent 2007;35:583-587.
-
16Odian G. Introduction. In: Principles of Polymerization, 4th Edition. John Wiley & Sons, Inc.: Hoboken, USA; 2004.
-
17Bishara SE, Von Wald L, Olsen ME, Laffoon JF. Effect of time on the shear bond strength of glass ionomer and composite orthodontic adhesives. Am J Orthod Dentofacial Orthop 1999;116:616-620.
-
18Oliveira AS, Barwaldt CK, Bublitz LS,. Moraes RR Impact of bracket displacement or rotation during bonding and time of removal of excess adhesive on the bracket-enamel bond strength. J Orthod 2014;41:124-127.
-
19Gonçalves LS, Moraes RR, Ogliari FA, Boaro L, Braga RR, Consani S. Improved polymerization efficiency of methacrylate-based cements containing an iodonium salt. Dent Mater 2013;29:1251-1255.
-
20Artun J, Bergland S. Clinical trials with crystal growth conditioning as an alternative to acid-etch enamel pretreatment. Am J Orthod 1984;85:333-340.
-
21Kim D,. Stansbury JW Kinetic pathway investigations of three component photoinitiator systems for visible-light activated free radical polymerizations. J Polymer Science Part A: Polymer Chemistry 2009;47:887-898.
-
22Padon KS, Scranton AB. A mechanistic investigation of a three component radical photoinitiator system comprising methylene blue, N-methyldiethanolamine, and diphenyliodonium chloride. Journal of Polymer Science Part A: Polymer Chemistry 2000;38:2057-2066.
-
23Leung RL, Fan PL, Johnston WM. Post-irradiation polymerization of visible light-activated composite resin. J DentRes 1983;62:363-365.
-
24Burtscher P. Stability of radicals in cured composite materials. Dent Mater1993;9:218-221.
-
25Mohamad D, Young RJ, Mann AB, Watts DC. Postpolymerization of dental resin composite evaluated with nanoindentation and micro-Raman spectroscopy. Arch Orofacial Scienc 2007;2:26-31.
Publication Dates
-
Publication in this collection
July 2014
History
-
Received
28 Feb 2014 -
Accepted
03 June 2014