Open-access Increased mechanical resistance in low-temperature ceramic blocks through geopolymerization*

Abstract

One of the challenges faced in constructions with ceramic materials is the low firing temperature, an inherent limitation in several industries. One solution to this problem is to reinforce these products with geopolymers formed by the alkaline activation of metakaolinite. This research is based on a factorial experimental design with the parameters: the firing temperature of the kaolinitic clay contained in the blocks, the molar concentration of KOH, and the curing temperature, aiming to analyze the efficiency of geopolymerization. The results show an increase in mechanical resistance for all geopolymerized specimens compared to non-geopolymerized specimens, with a notable increase of around 50% associated with low efflorescence. The developed prototypes allow for the possibility of industrial application, which would contribute to innovation and sustainability, highlighting the increase in mechanical resistance after geopolymerization at 700 °C, reaching more than 12 MPa, as indicated in the ISO 10545 standard for porous ceramic tilings.

Keywords:
ceramic masonry; geopolymerized ceramics; alkaline activation; potassium hydroxide; sustainability

INTRODCTION

Ceramic blocks in structural masonry, whether reinforced or unreinforced, began to be introduced into the Brazilian construction market in the 1980 s, with the introduction of modular units and vertical holes that allowed installations to be installed without the usual openings in walls. However, it was from 1990 onwards that the study of structural masonry intensified, which proposed significant rationalization in construction methods, notably the adoption of 15 cm modulated blocks, precast stairs, and the use of dedicated equipment and tools. 1.

The construction industry has been seeking to develop and employ efficient technologies in housing construction, while also ensuring sustainability and environmental preservation, aiming to increase productivity and reduce waste and costs. Thus, construction with ceramic structural masonry has gained prominence due to several advantages, such as savings in steel, concrete, and formwork when compared to buildings traditionally constructed with reinforced concrete. It also provides benefits such as durability, resistance to aggressive agents, fire resistance, incombustibility, thermal insulation, good watertightness, the possibility of being assembled into various forms, reusability, and broad acceptance by society 2.

It should be emphasized that the implementation of structural masonry presupposes a quality standard for ceramic blocks that is much higher than that inherent in blocks intended for enclosing masonry. In this context, it is emblematic to note that the vast majority of small-scale red ceramic industries in Brazil, generally small family-based businesses, use outdated production techniques, with a technological delay of approximately fifty years, and a lack of effective control of process variables, which is reflected in the production of low-quality pieces with firings below 900 °C. Firings at 600 °C are common, in which the complete loss of hydroxyls in clay minerals occurs, having active sites for the formation of new bonds, but with low mechanical resistance, since only from 900 °C onwards are more resistant phases and vitreous phases formed. 3), (4.

A type of structural masonry construction that became popular in the 1970 s in Pernambuco, Brazil, is the box-shaped building. This name refers to the box-like shape of the buildings, which are built without the use of reinforced concrete, rising wall upon wall, with “resistant masonry” - without beams and pillars. With up to four stories, to avoid the use of elevators, these buildings also became popular due to the lobbying of a ceramics union that existed in the state, offering reduced costs and streamlined construction 5.

However, due to construction quality issues, as well as issues such as groundwater, heavy rains, and flooding, the materials used were further degraded. Problems began to emerge in the 1990 s, when several box-shaped buildings in Greater Recife (capital of Pernambuco, Brazil) collapsed. According to a survey by the Pernambuco Institute of Technology (ITEP), released in 2023, approximately 1,000 box-shaped buildings in the Recife Metropolitan Region are in a compromising condition, with cracks, structural movement, and even risk of collapse 5.

One solution to this problem of poorly fired ceramic blocks is to improve mechanical resistance through geopolymerization, since low firing temperatures ceramics contain metakaolinite, an amorphous aluminosilicate, which is one of the geopolymer formers when activated by alkaline elements 6.

During ceramic firing, at approximately 700 °C, almost all of the hydroxyl groups in the kaolinite present in the kaolin are removed, changing the aluminum coordination number from VI to IV, reducing the stability of the kaolinite, forming metakaolinite, which is an amorphous phase due to the release of water molecules that were part of the kaolinite, destroying the ordered arrangement that characterizes its crystalline structure. A similar process occurs with other clay minerals, as seen in reactions (1) and (2) below 7:

Al 2 O 3 · 2 SiO 2 · 2 H 2 O → Al 2 O 3 · 2 SiO 2 + 2 H 2 O (A)

Al 2 Si 2 O 5 OH 4 → Al 2 O 3 · 2 SiO 2 + 2 H 2 O kaolinite metakaolinite (B)

Thus, it can be stated that geopolymers are formed by chains or rings with Si+4 and Al+3 in coordination number IV with oxygen. The fact that aluminum exhibits coordination number IV with oxygen creates an unbalanced negative charge, and therefore, the presence of metal cations (K+, Na+) occupying the cavities of the structure (sialate) is essential to neutralize this excess negative charge. Geopolymers have a chemical composition similar to zeolites, but with structures ranging from amorphous to semicrystalline.

Silica (SiO2) and alumina (Al2O3), constituents of aluminosilicates, react with each other in a strongly alkaline environment and, organizing alternately in three dimensions, give rise to a sialate network, which consists of SiO4 and AlO4 tetrahedra alternately linked through the sharing of oxygen atoms. The various sialate networks alternately link through polycondensation reactions and give rise to the polymeric units that form geopolymers. A sialate network is, ultimately, the monomer of a polymeric structure. Geopolymers are inorganic polymers, generated by polycondensation with subsequent hardening, like cements 8.

The polycondensation that leads to geopolymerization involves initial dissolution, in which the alkaline solution not only hydrolyzes the surface of the raw material particles (aluminosilicate) but also dissolves a small amount of Al and Si. These react with the already dissolved ions and polymerize, through condensation reactions, forming a gel that is transformed into the final structure 9. Alkaline-activated materials can be used as cements when the precursor has a Si/Al atomic ratio between 1 and 3, such as metakaolinite 10.

The solid obtained with geopolymer cement is very different from that obtained by hydrating Portland cement. Its structure is massive, with no defined morphology, and its composition is similar to that of rocks. Furthermore, there is no formation of calcium hydroxide, and C-S-H is virtually absent. The solid is composed primarily of amorphous silico-aluminates, and there are no phases that stand out under electron microscopy.

Sodium hydroxide (NaOH), potassium hydroxide (KOH), and sodium silicate (Na2SiO3) have been used as activators of the alkaline reaction of metakaolinite, and processing parameters that interfere with the properties of the geopolymer include the sintering temperature, the molar fraction of each activator, and the curing time and temperature 11.

Among the alkali metals, potassium hydroxide presents greater stability and ease of geopolymerization due to the larger size of the K+ ion when compared to Na+, providing greater mechanical resistance for comparison at the same molarity 12), (13. Thus, KOH becomes more reliable for statistical planning without the need for many characterization tests, given that it will tend to increase resistance with less carbonation than NaOH (less efflorescence), for variations in molarity and curing time.

To evaluate all these factors in relation to the flexural resistance of ceramic specimens, a statistical design was performed using firing temperature, KOH molar concentration, and curing time as variables for optimal flexural resistance. Thus, the study aims to contribute to both applied science and the construction industry in the production of higher-quality, more durable ceramic blocks even at low firing temperatures. This contributes to sustainability by reducing energy consumption and avoiding the use of cement, reducing CO2 emissions, and supporting the development of the ceramics industry.

MATERAILS AND METHODS

Materials

The experimental work aimed at this investigation was developed at the Campus of the Federal University of Campina Grande, state of Paraíba, more specifically at the Technical Materials Laboratory -LTM The clay mass was selected in the municipality of Camaragibe - PE, Potassium hydroxide (KOH) PA 85%, Synth, Diadema-SP, Brazil was used as an alkaline agent to activate the metakaolinite, forming the geopolymer. Of the alkali metals most used for geopolymerization, potassium hydroxide has certain advantages such as favoring the formation of oligomers with Al, since Al(OH)- binds more easily with the K+ ion, which is larger than the Na+ ion. Furthermore, K+ requires a smaller hydration sphere than Na+, allowing denser polycondensation reactions, and is also more basic. Thus, precursors linked with KOH have greater mechanical resistance than precursors with NaOH 12), (13.

Clay characterization

Regarding the characterization of the clay used, Table I indicates the chemical composition of the studied mass, carried out using X-ray fluorescence equipment, Shimadzu EDX720, which shows that, as main constituents, silica and alumina appear, in the SiO2/Al2O3 ratio between 1 and 3, a fact that makes geopolymerization viable if alkaline reactions are provoked 10.

Table I
Chemical composition of the clay used.

The particle size distribution was determined by laser diffraction (Cilas, model 1064LD, Orléans, France). The thermal behaviors were evaluated by thermogravimetry (TG)/derivative thermogravimetry (DTG) (DTG Shimadzu, model TA 60H, Kyoto, Japan) and differential thermal analysis (DTA) (Instrumentec BP, model RB-3000, Campinas, Brazil), with a heating rate of 12 °C/min, under an air atmosphere and using calcined aluminum oxide (Al2O3).

The analysis of the variation in the particle dimensions of the clay used allowed the evaluation of its parameters Cu ≈ 15 (uniformity coefficient) and Cc ≈ 0.82 (curvature coefficient), which allows it to be classified as “poorly graded, with medium to “ununiform” granulometry”19. The analysis of the granulometric curve also indicated a clay content ≈ 30%.

When researching the moisture content of an industrial mass to be used in the production of ceramic samples by extrusion, this physical index (moisture) must generate consistency indices (CI) between 0.50 and 0.75 (average state of cohesion), as indicated in Table II. In this work, when molding the ceramic prototypes, the mass was manipulated at a humidity level that generated a CI ≈ 0.75. These results were obtained with the aid of Casagrande’s apparatus in accordance with ABNT NBR 6459 (Soil - Determination of the Liquid Limit).

Table II
Clay workability defined from CI.

Figure 1 indicates the thermal transformations of the “raw” mass intended for the production of ceramic prototypes, through the DTA performed on the BP equipment model RB-300. The large endothermic peak near 100 °C indicates the loss of free water and has no effective correlation with the mineralogical configuration of the analyzed material. The exothermic peak close to 300 °C is the latter, constituting a strong indication of the dissociation of aluminum hydroxide, which, in fact, is present in significant content, as detected by chemical analysis. The exothermic peak close to 580 °C stands out, characteristic of the loss of water due to the decomposition of the hydroxide, and the endothermic peak close to 900 °C, indicative of the nucleation of mullite. A total mass loss of 9% is observed, which corresponds mainly to the accumulation of free and adsorbed water losses, as well as the loss of kaolinite hydroxyls.

Figure 1:
DTA and TG of the mass used in the production of the prototypes.

Methods

The clay was stored in containers and moistened to determine the consistency index and subsequently moistened to make it compatible with extrusion molding in one meter of length (Verdéz monoblock extruder. Ref. 051, Fab. 1999, series 0023) as showed in Figure 2, resulting in filaments of varying dimensions of 50 mm x 10 mm x 10 mm which were fired in suitable furnaces and were submerged in the alkaline solutions (activating agents) for a period of twenty-four hours. KOH was prepared as a solution in water, using 70 mL of water for each gram of KOH. After which they remained for another twenty-four hours in the open air, from when curing began; this occurred over the course of five days, in a controlled atmosphere, inside an oven at the appropriate temperature as seen in Figure 2 below.

Figure 2:
Some steps in the processing of test specimens.

Once the curing stage was completed, the prototypes were subjected to water absorption analysis, being submerged for 24 h, checking the dry and wet masses and the flexural resistance test at three points, and followed the methodology indicated by ASTM C 1161 (1994) 14. The rupture of the mentioned prototypes occurred with the use of the Shimadzu universal machine, model AG-X 50 KN, at a flexural speed of 0.05 mm/min and 40 mm for length (10% of 50 mm). At the end of the experimental procedure, test specimens were separated to evaluate efflorescence, initially being checked only with humidity. The ceramic test specimens were subjected to a qualitative verification of efflorescence, which was carried out according to the ASTM C 67 15 “modified” test standard, with samples chosen based on the maximum molarity and curing temperature parameters of 700 °C and 900 °C (700G+ and 900G+). Initially, the so-called premature efflorescence was evaluated, which is the type that occurs only in the presence of moisture. After this test, the efflorescence of salts after immersion in distilled water for 7 days is compared with other test specimens that were not subjected to immersion. When efflorescence occurs, some of the test specimens subjected to immersion will show characteristic stains from salt deposition.

For the experimental planning, the factors of firing temperature, molar concentration, and curing temperature were analyzed, evaluating the flexural resistance as a response. Based on previous studies like Ramos 16 and Costa et al. 11, linear relationships are assumed between increasing molarity and increasing temperature, eliminating the need for star-type designs with quadratic relationships. The software for Design of Experiments used was Statistica 7 (developed by StatSoft, Inc. in 2004). Thus, with three factors, varying two levels with a central point, the chosen design was the 2³ factorial design with a central point, thus having 8 assays plus 4 assays at the central point to reduce errors and improve statistical reliability, with 95% confidence, having low data dispersion, with ten samples used for each trial.

The transmission of the thermal energy in question must preserve amorphous phases inside the ceramic prototypes, which is why temperatures must be higher than 600 °C 17. To be able to form metakaolinite and reach a maximum close to 900 °C 18, otherwise, triggering of a metakaolinite crystallization process would prevent the desired polymerization phenomenon. Table III below presents the experimental design so that the code +1 represents the upper limit and -1 the lower limit, for each factor, with the complete design presented in Table IV.

Table III
Upper and lower limit values for the 3 factors of the experimental design

Table IV
Complete 2³ factorial design with central points.

For samples characterization, X-ray Fluorescence (XRF) and X-ray Diffraction (XRD) were relative to the temperatures of 700 °C and 900 °C at the maximum molar concentrations of KOH and curing temperatures, designated 700 G+ and 900 G+, respectively. These were compared with the non-geopolymerized specimens at the same temperatures, designated 700 N and 900 N, for the temperatures of 700 °C and 900 °C, respectively.

The chemical characterizations and mineral phases of the raw materials were performed using X-ray fluorescence (EDX 720 - Shimadzu) and X-ray diffraction (XRD600 - Shimadzu), using CuKα radiation (λ = 1.54 Å), operated at 40 kV and 30 mA, in the angular range of 2θ from 5 to 60° and a step size of 0.02°.

RESULTS AND DISCUSSIONS

As reference values for mechanical resistance, we have the test specimens fired at 700 °C, 800 °C, and 900 °C, with the data presented in Table IV. It is important to highlight two main factors for the increase in mechanical resistance, which are the densification of the test specimen with sintering, which promotes atomic diffusion between the particles, reducing the size of the pores, and the formation of new resistance phases, among them some vitreous phases that fuse and fill the cavities. Thus, to evaluate the increase in mechanical resistance due to the action of geopolymerization, it must be compared at each temperature. Regarding water absorption, for all test specimens, values below those suggested by researchers were obtained, as per Souza Santos (1989), who indicates that ceramic masses after firing must present water absorption of less than 25% and a modulus of rupture greater than 5 MPa 20. The water absorption values at temperatures of 700 °C and 800 °C were greater than 10%, according to the ISO 10545:2020 standard 21, and less than 25% according to Santos 20

In the work of Botelho (2024) 22 that evaluates geopolymerization in kaolinitic clay at 700 °C, 800 °C and 900 °C, it is possible to observe the amorphous region in the XRD characteristic of metakaolinite at all these temperatures, with no noticeable difference, observing only the greater formation of crystalline phases such as mullite and the decrease in phases with greater humidity such as muscovite that has hydroxyls.

According to Figure 3a, it can be concluded that the sintering temperature, reagent concentration, and curing time factors presented adequate statistical values, all greater than the p parameter, which is 0.05. That is, with 95% significance, all parameters are statistically significant, as evaluated in the ANOVA table. In Figure 3b, it can be seen that the predicted and observed values are close to linearity, indicating that the planning is adequate, without the need to evaluate the extra points, called star points, contained in the composite factorial design.

Figure 3:
Pareto chart (a) and graph of predicted vs. observed values.

Table VI presents the flexural resistance results for all temperatures. An increase in mechanical resistance is observed with increasing curing time and alkaline agent concentration, with a small change in the contour line profile as the temperature is increased. In other words, for higher temperatures, shorter curing times and KOH concentrations are required to obtain the highest flexural resistance values. Considering the highest curing temperature (80 °C) as shown in Figure 1a, even at the lowest KOH concentrations, it is possible to obtain flexural resistance values higher than the reference value, without geopolymerization (10.03 MPa).

Table V
Flexural resistance results for each temperature of non-geopolymerized test specimens.

Table VI
Flexural resistance results for each planning assay.

Figure 4:
Response surfaces and level curve for the optimal curing and molarity parameters.

Evaluating the relationship between molarity and firing temperature for the maximum curing temperature (80 °C) as shown in Figure (a), since it is at the optimum point, that is, at the curing temperature with the highest flexural resistance value, it is observed that for low molarities, high firing temperatures are required to obtain higher resistances and with increasing molarity, lower firing temperatures are required to obtain even higher resistances Since the response surface is flat, the data are better verified in contour plots or level curves (Figure 3b), which are used for the remaining analyses.

In Figures c and d, using the same justification as in Figure a, for maximum molarity, the influence of temperature is greater than the curing time, since increasing the temperature promotes an increase in resistance, even for lower curing temperatures, with the optimum value at 80 °C of curing temperature and 900 °C of sinterization temperature. Although the graph shows an increase in resistance above 900 °C, it is worth noting that metakaolinite crystallization is already possible, thus reducing geopolymer production and causing a decrease in resistance.

Evaluating the relationship between molarity and curing temperature for each firing temperature, as shown in Figure 5, we observe that at 700 °C, increasing molarity has a greater effect than increasing curing temperature. However, as the temperature increases to 800 °C, a higher curing temperature is required to achieve a more effective increase in resistance. Because the statistical analysis is highly reliable, we can evaluate at temperatures where no testing was performed, such as at 850 °Cthrough data interpolation, observing the need for higher curing temperatures until reaching 900 °C, where the contour lines are more “horizontal.” That is, for low molarities, a higher curing temperature is required to achieve an effective increase in mechanical resistance.

Figure 5:
Level curves for each firing temperature.

Comparing the resistance values obtained for each firing temperature, as per Table VI, there is an increase in percentage for each optimum point (80 °C curing temperature at 2.82 molarity) of 10.26% for 700 °C and 54.36% for 900 °C. This higher value of increase in mechanical resistance at the temperature of 900 °C may be associated with two main factors: the densification of the geopolymer itself, which is porous 23, and also the increase in its quantity, since it is possible to continue polymerization up to 900 °C.

All test specimens did not present the so-called premature efflorescence, presenting a slight occurrence of efflorescence only after having been immersed in distilled water for 7 days, as observed in Figure 6. Due to the low efflorescence observed with minimal degradation, characteristic of crystal formation, it was neither possible nor necessary to perform a quantitative evaluation based on the percentage of area with efflorescence compared to the total area of the test specimen according to ASTM C 67 15.

Figure 6:
Efflorescence test results on specimens 700G+ (a) and 900G+ (b).

The presence of little efflorescence indicates that most of the KOH participated in the chemical reactions for the formation of geopolymers, with no excess of salts visualized in the efflorescence, resulting from the reaction of free alkalis with carbon dioxide from the atmosphere (carbonation), as explained in the research by Longhi 24. While the test specimens that were not geopolymerized (Figure 7) showed considerable occurrence of efflorescence at 700 °C and slight occurrence of efflorescence at 900 °C, this must be due to the presence of alkali metal ions such as Na+ and K+ in the clay itself, which, when in excess, promote efflorescence.

Figure 7:
Result of the efflorescence test on bodies without geopolymerization of 700N (a) and 900N (b).

Comparing the efflorescences, it can be assumed that the alkaline activation with potassium hydroxide contributed to the formation of the geopolymer, including facilitating the reaction of other salts present in the non-geopolymerized specimen, taking as reference several studies such as the use of potassium hydroxide as opposed to sodium hydroxide by Najaki Kani et al. 25 and more recently by 26. This may be possible because potassium hydroxide has stronger chemical bonds with the aluminum silicate gel structure 25.

Furthermore, potassium carbonate (K2CO3) has greater solubility than sodium carbonate (Na2CO3), forming fewer crystals that migrate to the surface of the material, causing efflorescence 27, reinforcing the statement by Lonhi et al. that the use of K+ is effective in reducing the formation of visible efflorescence 28. The moisture content of the material and curing conditions must also be taken into account, as this can facilitate the migration of alkalis through the pore structure of the material to the surface, interacting with the air and forming carbonates (efflorescence) 29), (30), (31

The low efflorescence presented by the test specimens makes them more viable for use in structural masonry, since efflorescence can worsen even with the time of exposure of the ceramic, as verified in the research by Costa et al., which showed an increase in the efflorescence of alkalized ceramic test specimens up to 60 days of exposure to the environment 11. It has been proven that geopolymerized materials with low or no efflorescence have high durability, with a durability of 30 years being verified by Provis 32.

Table VII presents the results of the X-ray Fluorescence analyses performed for two geopolymerized samples under maximum molarity and curing conditions. Calculating the SiO2/Al2O3 molar ratio based on the XRF result according to Table VII yields a value of 1.30. Although this is a lower ratio than the recommended 1:5.5 or 1:6.5 31, the potassium ion can react more easily with the aluminum ion, facilitating geopolymerization 34) (35.

Table VII
X-ray Fluorescence results for geopolymerized samples.

The potassium oxide value increased considerably from 0.09% in the raw clay to 5.3%, representing a K2O/Al2O3 and K2O/SiO2 ratio of 0.15 and 0.12, which were also lower than indicated in the literature 3. However, it is important to emphasize that high K2O values can increase the efflorescence phenomenon in the ceramic specimens, proving to be suitable for this work, since there was no “premature” efflorescence and low efflorescence was obtained after immersion in water.

In Figure 8, after processing the curves to better identify the peaks indicating crystallinity, it is possible to observe the shift of some phases from 700 N to 700 G+, such as biotite, potassium feldspar (microline), and even albite. At 900 °C, the disappearance of some hydroxyl-containing phases, such as biotite, is expected, but a decrease in crystalline peaks also occurs with alkaline activation, forming the geopolymer in the 900 G+ curve. Analysis of these XRD graphs confirms the influence of geopolymers on the increased mechanical resistance, as demonstrated in the tests.

Figure 8
: Identification of the crystalline phases with JCPDS codes of the analyzed samples. B - Biotite (96-900-0844); Q - Quartz (01-086-2237); M - Microline (potassium feldspar - 00-022-0687); A - Albite (00-010-0393).

CONCLUSIONS

Based on the proposed results, it can be concluded that the statistical planning was adequate, without the need for axial points, since the upper and lower limits of each factor were carefully analyzed to ensure a response within the desired range. The combined evaluation of the 3 parameters promoted the best results for the highest molarity, the highest curing temperature, and the highest sintering temperature. Among the parameters evaluated, temperature is the factor that most influences the response (flexural strength), followed by molarity and curing temperature. Potassium hydroxide showed good stability in all tests, with low efflorescence, increasing resistance with increasing molarity up to approximately 3 mol/L.

The geopolymerized product demonstrated efficient application in ceramic coating, standing out at 700 °C for achieving the necessary mechanical resistance only after geopolymerization, highlighting its importance. For industrial production, lower temperatures may be even more viable, considering the energy savings and the resistance gains obtained with geopolymerization.

ACKNOWLEDGMENTS

The authors would like to thank the National Council for Scientific and Technological Development - CNPq, for the financial support granted to the research projects (nº 407848/2022-3 and 309771/2021-8), the Financing Agency for Studies and Projects - FINEP (project no. 01.22.0251.00), and the Paraíba State Research Support Foundation - FAPESQ (Announcement 06/2021, project no. 3064/202). They would also like to thank the companies that provided the waste used in this study, as well as the Federal University of Campina Grande - UFCG, for the institutional support and financial support.

DATA AVAILABILITY

The data that support the findings of this study are available from the corresponding author upon reasonable request.

REFERENCES

  • 1 G. Mohamad, Construções em Alvenaria Estrutural - Material, projetos e desempenho, 3rd ed. 2025.
  • 2 D. R. B. Lima, L. R. Meira, and A. B. Dantas, “Alvenaria Estrutural E Método 3D: Comparativo De Custo para construção de habitações de interesse social,” vol. 14, Jan. 2020.
  • 3 S. N. Monteiro and C. M. F. Vieira, “Solid state sintering of red ceramics at lower temperatures,” Ceram Int, vol. 30, no. 3, pp. 381-387, 2004, doi: https://doi.org/10.1016/S0272-8842(03)00120-2
    » https://doi.org/10.1016/S0272-8842(03)00120-2
  • 4 M. S. S. A. Savazzini-Reis, M. S. Silva, A. Savazzini-Reis, and M. S. Silva, “Análise do Desempenho de Blocos Cerâmicos Produzidos na Região de Colatina-ES,” Cerâmica Industrial, vol. 22, no. 3, pp. 39-46, Sep. 2017, doi: 10.4322/CERIND.2017.018.
    » https://doi.org/10.4322/CERIND.2017.018
  • 5 G1.Globo, “Prédio que desabou no Grande Recife é do tipo ‘caixão’, construção proibida há 20 anos; entenda,” 2025. Accessed: Jul. 08, 2025. [Online]. Available: Available: https://g1.globo.com/pe/pernambuco/noticia/2025/05/06/predio-que-desabou-no-grande-recife-e-do-tipo-caixao-construcao-proibida-ha-20-anos-entenda.ghtml
    » https://g1.globo.com/pe/pernambuco/noticia/2025/05/06/predio-que-desabou-no-grande-recife-e-do-tipo-caixao-construcao-proibida-ha-20-anos-entenda.ghtml
  • 6 A. V. Lot, F. G. Melchiades, and A. O. Boschi, “Influência das Características de Metacaulins no Desempenho de Geopolímeiros,” Cerâmica Industrial , vol. 20, no. 3, pp. 35-41, 2015, doi: 10.4322/cerind.2015.017.
    » https://doi.org/10.4322/cerind.2015.017
  • 7 P. Souza Santos, Ciência e tecnologia das argilas, 2nd ed., vol. 1, 2, 3. Edgard Blucher, 1992.
  • 8 J. Davidovits, “Geopolymers: Man-made rock geosynthesis and the resulting development of very early high strength cement,” J. Mater. Edu., vol. 16, pp. 91-137, Jan. 1994.
  • 9 J. G. S. Van Jaarsveld, J. S. J. Van Deventer, and L. Lorenzen, “Factors affecting the immobilization of metals in geopolymerized flyash,” Metallurgical and Materials Transactions B, vol. 29, no. 1, pp. 283-291, 1998, doi: 10.1007/s11663-998-0032-z.
    » https://doi.org/10.1007/s11663-998-0032-z
  • 10 J. Davidovits, “30 Years of Successes and Failures in Geopolymer Applications. Market Trends and Potential Breakthroughs,” in Geopolymer 2002 Conference, Melbourne, Australia: Conference Proceedings, Oct. 2002.
  • 11 F. P. da Costa, I. M. T. Bezerra, J. V. Fernandes, A. M. Rodrigues, R. R. Menezes, and G. de A. Neves, “Durability of Sustainable Ceramics Produced by Alkaline Activation of Clay Brick Residue,” Sustainability, vol. 13, no. 19, p. 10931, Oct. 2021, doi: 10.3390/su131910931.
    » https://doi.org/10.3390/su131910931
  • 12 J. W. Phair and J. S. J. Van Deventer, “Effect of silicate activator pH on the leaching and material characteristics of waste-based inorganic polymers,” Miner Eng, vol. 14, no. 3, pp. 289-304, 2001, doi: https://doi.org/10.1016/S0892-6875(01)00002-4
    » https://doi.org/10.1016/S0892-6875(01)00002-4
  • 13 J. W. Phair and J. S. J. van Deventer, “Characterization of Fly-Ash-Based Geopolymeric Binders Activated with Sodium Aluminate,” Ind Eng Chem Res, vol. 41, no. 17, pp. 4242-4251, Aug. 2002, doi: 10.1021/ie010937o.
    » https://doi.org/10.1021/ie010937o
  • 14 ASTM, Standard Test Method for Flexural Strength of Advanced Ceramics at Ambient Temperature. American Society for Testing and Materials, 1996.
  • 15 ASTM. C67-08. Standard Test Methods for Sampling and Testing Brick and Structural Clay Tile (Efflorescence Test). ASTM International, 2008.
  • 16 S. de O. Ramos.Ativação alcalina em peças de cerâmica vermelha. Dissertação de Mestrado, UFCG. Campina Grande, Paraíba, Brasil, 2010.
  • 17 B. B. Sabir, S. Wild, and J. Bai, “Metakaolin and calcined clays as pozzolans for concrete: a review,” Cem Concr Compos, vol. 23, no. 6, pp. 441-454, 2001, doi: https://doi.org/10.1016/S0958-9465(00)00092-5
    » https://doi.org/10.1016/S0958-9465(00)00092-5
  • 18 R. Cao, Z. Fang, M. Jin, and Y. Shang, “Study on the Activity of Metakaolin Produced by Traditional Rotary Kiln in China,” Minerals, vol. 12, no. 3, 2022, doi: 10.3390/min12030365.
    » https://doi.org/10.3390/min12030365
  • 19 W. Kriven, J. L. Bell, and M. Gordon, “Microstructure and Microchemistry of Fully-Reacted Geopolymers and Geopolymer Matrix Composites,” Ceramic Transactions, vol. 153, pp. 227-250, Jan. 2004.
  • 20 P. de S. Santos, Ciência e Tecnologia de Argilas: Vol 1, Vol 2 e Vol 3. Edgard Blucher, 1992.
  • 21 ABNT ISO 10545-4:2020. Placas cerâmicas - Parte 4: Determinação da carga de ruptura e módulo de resistência à flexão. São Paulo: Associação Brasileira de Normas Técnicas, 2020.
  • 22 J. A. Botelho, “Estudo do processo de calcinação do caulim para produção de geopolímeros,” Ananindeua - Pará Brasil., 2024. Accessed: Jul. 27, 2025. [Online]. Available: Available: https://bdm.ufpa.br/items/69f26db3-775c-4d1f-a393-733b226bae7f
    » https://bdm.ufpa.br/items/69f26db3-775c-4d1f-a393-733b226bae7f
  • 23 A. van Riessen, E. Jamieson, H. Gildenhuys, R. Skane, and J. Allery, “Using XRD to Assess the Strength of Fly-Ash- and Metakaolin-Based Geopolymers,” Materials, vol. 18, no. 9, p. 2093, May 2025, doi: 10.3390/ma18092093.
    » https://doi.org/10.3390/ma18092093
  • 24 M. A. Longhi, Z. Zhang, E. D. Rodríguez, A. P. Kirchheim, and H. Wang, “Efflorescence of Alkali-Activated Cements (Geopolymers) and the Impacts on Material Structures: A Critical Analysis,” Front Mater, vol. Volume 6-2019, 2019, doi: 10.3389/fmats.2019.00089.
    » https://doi.org/10.3389/fmats.2019.00089
  • 25 E. Najafi Kani, A. Allahverdi, and J. L. Provis, “Efflorescence control in geopolymer binders based on natural pozzolan,” Cem Concr Compos , vol. 34, no. 1, pp. 25-33, 2012, doi: https://doi.org/10.1016/j.cemconcomp.2011.07.007
    » https://doi.org/10.1016/j.cemconcomp.2011.07.007
  • 26 J. K. De Ré, A. L. Sokolovski, and S. C. Vanzetto, “Avaliação do uso do hidróxido de potássio em geopolímeros visando à prevenção de formação de eflorescência,” Ambiente Construído, vol. 25, 2025, doi: 10.1590/s1678-86212025000100785.
    » https://doi.org/10.1590/s1678-86212025000100785
  • 27 F. Škvara, L. Kopecky, L. Myskova, V. Smilauer, L. Alberovska, and L. Vinsova, “Aluminosilicate polymers - influence of elevated temperatures, efflorescence,” Ceramics, vol. 53, no. 4, pp. 276-282, 2009.
  • 28 M. A. Longhi, E. D. Rodríguez, B. Walkley, Z. Zhang, and A. P. Kirchheim, “Metakaolin-based geopolymers: Relation between formulation, physicochemical properties and efflorescence formation,” Compos B Eng, vol. 182, p. 107671, 2020, doi: https://doi.org/10.1016/j.compositesb.2019.107671
    » https://doi.org/10.1016/j.compositesb.2019.107671
  • 29 A. Saludung, T. Azeyanagi, Y. Ogawa, and K. Kawai, “Effect of silica fume on efflorescence formation and alkali leaching of alkali-activated slag,” J Clean Prod, vol. 315, p. 128210, 2021, doi: https://doi.org/10.1016/j.jclepro.2021.128210
    » https://doi.org/10.1016/j.jclepro.2021.128210
  • 30 A. Wang et al., “The Durability of Alkali-Activated Materials in Comparison with Ordinary Portland Cements and Concretes: A Review,” Engineering, vol. 6, no. 6, pp. 695-706, 2020, doi: https://doi.org/10.1016/j.eng.2019.08.019
    » https://doi.org/10.1016/j.eng.2019.08.019
  • 31 N. A. M. Sani, Z. Man, R. M. Shamsuddin, K. A. Azizli, and K. Z. K. Shaari, “Determination of Excess Sodium Hydroxide in Geopolymer by Volumetric Analysis,” Procedia Eng, vol. 148, pp. 298-301, 2016, doi: https://doi.org/10.1016/j.proeng.2016.06.621
    » https://doi.org/10.1016/j.proeng.2016.06.621
  • 32 J. L. Provis et al., “Will Geopolymers Stand the Test of Time?,” in Developments in Porous, Biological and Geopolymer Ceramics, Hoboken, NJ, USA: John Wiley & Sons, Inc., 2008, pp. 235-248. doi: 10.1002/9780470339749.ch22.
    » https://doi.org/10.1002/9780470339749.ch22
  • 33 D. Khale and R. Chaudhary, “Mechanism of geopolymerization and factors influencing its development: a review,” J Mater Sci, vol. 42, no. 3, pp. 729-746, 2007, doi: 10.1007/s10853-006-0401-4.
    » https://doi.org/10.1007/s10853-006-0401-4
  • 34 Q. Yang, C. A. Davy, J. Sarazin, S. Bourbigot, and G. Fontaine, “Effect of cation in sodium/potassium-based geopolymer coatings for the fire protection of steel structures,” Ceram Int , vol. 51, no. 4, pp. 4532-4548, 2025, doi: https://doi.org/10.1016/j.ceramint.2024.11.428
    » https://doi.org/10.1016/j.ceramint.2024.11.428
  • 35 R. Khan, S. Iqbal, M. Soliyeva, A. Ali, and N. Elboughdiri, “Advanced clay-based geopolymer: influence of structural and material parameters on its performance and applications,” RSC Adv, vol. 15, no. 16, pp. 12443-12471, 2025, doi: 10.1039/D4RA07601J.
    » https://doi.org/10.1039/D4RA07601J

*

Paper presented at the 69th CBC (https://abceram.org.br/69cbc/)

AE:

Daniel Zanetti de Florio

Publication Dates

  • Publication in this collection
    21 Sept 2026
  • Date of issue
    2026

History

  • Received
    15 Aug 2025
  • Reviewed
    31 Jan 2026
  • Reviewed
    19 Mar 2026
  • Accepted
    03 June 2026
location_on
Associação Brasileira de Cerâmica Av. Prof. Almeida Prado, 532 - IPT - Prédio 36 - 2º Andar - Sala 03 , Cidade Universitária - 05508-901 - São Paulo/SP -Brazil, Tel./Fax: +55 (11) 3768-7101 / +55 (11) 3768-4284 - São Paulo - SP - Brazil
E-mail: ceramica.journal@abceram.org.br
rss_feed Stay informed of issues for this journal through your RSS reader
Go to top