Abstract
This study investigated the effect of phytic acid (IP6) in different concentrations and application times on microtensile bond strength (µTBS) and interfacial integrity of universal adhesive to deep dentin. Flat deep dentin surfaces of 48 human molars were either etched with 37% phosphoric acid (PA) for 15 sec (control); or received no acid treatment and universal adhesive was applied directly in a self-etch mode (SE); or divided according to IP6 concentration (C) into two main groups: C1, 0.5%, and C2, 1%. Specimens of IP6 groups were further subdivided into three subgroups according to application time of IP6 (T) where; T1, 15 sec; T2, 30 sec and T3, 60 sec. Single Bond Universal Adhesive was then applied and resin composite blocks were built-up. Forty Specimens were then sectioned to produce resin/dentin beams that were used for µTBS testing using a universal testing machine. The remaining eight specimens were sectioned into slabs that were immersed into ammonical silver nitrate solution and nanoleakage was observed using a field emission scanning electron microscope (FE-SEM). The results showed that the application of IP6 in 0.5% and 1% produced significantly higher µTBS and less nanoleakage compared to PA and SE groups. Also, the application of IP6 for 60 sec recorded the highest µTBS and the lowest nanoleakage followed by 30 sec, and 15 sec respectively. Therefore, conditioning of deep dentin with IP6 enhances µTBS and interfacial integrity of universal adhesive to deep dentin in comparison to PA etching or using the universal adhesive in SE mode.
Key Words:
deep dentin; microtensile bond strength; phytic acid; phosphoric acid; universal adhesive
Resumo
Este estudo investigou o efeito do ácido fítico (IP6) em diferentes concentrações e tempos de aplicação na resistência da ligação microtensiva (µTBS) e na integridade interfacial do adesivo universal à dentina profunda. As superfícies planas de dentina profunda de 48 molares humanos foram preparadas com ácido fosfórico (PA) a 37% durante 15 seg. (controlo); ou não receberam tratamento ácido e o adesivo universal foi aplicado diretamente em modo de auto-adesivo (SE); ou dividido de acordo com a concentração de IP6 (C) em dois grupos principais: C1, 0,5%, e C2, 1%. Os espécimes dos grupos IP6 foram ainda subdivididos em três subgrupos de acordo com o tempo de aplicação do IP6 (T) em que; T1, 15 seg; T2, 30 seg e T3, 60 seg. Aplicou-se então Single Bond Universal Adhesive e construíram-se blocos compostos de resina. Quarenta espécimes foram então seccionados para produzir feixes de resina/dentina que foram usados para testes µTBS usando uma máquina de testes universal. Os restantes oito espécimes foram seccionados em placas que foram imersas em solução amoniacal de nitrato de prata e observou-se uma nano-infiltração utilizando um microscópio eletrônico de varrimento de emissões de campo (FE-SEM). Os resultados mostraram que a aplicação de IP6 em 0,5% e 1% produziu µTBS significativamente mais elevado e menos nano-infiltração em comparação com os grupos PA e SE. Além disso, a aplicação de IP6 durante 60 seg registou o µTBS mais alto e o mais baixo de nano-infiltração seguido de 30 seg, e 15 seg respectivamente. Portanto, o condicionamento da dentina profunda com IP6 melhora o µTBS e a integridade interfacial do adesivo universal à dentina profunda em comparação com a gravação de PA ou utilizando o adesivo universal no modo SE.
Introduction
Resin composite bond strength to dentin has an important role in restoration success. Bonding mechanism of dentin is different from enamel due to basic differences in their organic and inorganic material 11. Sharafeddin F, Nouri H, Koohpeima F. The effect of temperature on shear bond strength of clearfil SE bond and adper single bond adhesive systems to dentin. J Dent Shiraz Univ Med Sci 2015; 16(1):10-6.. Dental enamel is highly mineralized tissue composed of 85 vol% minerals and a low percentage of protein, lipid and water 22. Featherstone JD, Lussi A. Understanding the chemistry of dental erosion. Monogr. Oral Sci2006; 20: 66-76. while dentin is composed of approximately 50 vol% mineral phase, 30 vol% collagen and 20 vol% water 33. Pashley DH, Tay FR, Breschi L, Tjäderhane L, Carvalho RM, Carrilho M, et al. State of the art etch-and-rinse adhesives. Dent Mater2011; 27(1): 1-16.. Therefore, bonding to dentin represents a much greater challenge than to enamel 44. Akbarian S, Sharafeddin F, Akbarian G. Evaluation of the influence of three different temperatures on microleakage of two self-etch and one total-etch adhesives. J Contemp Dent Pract2015; 16(3): 178-82. especially in deeper dentin due to the decrease in inter-tubular dentin and the increase in tubular diameter as well as water content 55. Kinney JH, Balooch M, Marshall SJ, Marshall GW Jr, Weihs TP. Atomic force microscope measurements of the hardness and elasticity of peritubular and intertubular human dentin. J Biomech Eng1996; 118: 133-35..
Over the years, phosphoric acid (PA) etching has been used to enhance the substrate surface characteristics before the application of the adhesive system 66. Mosharrafian S, Afshar H, Farbod M , Baniameri Z. Effect of etching time and preparation on push-out bond strength of composite to intracanal dentin of primary anterior teeth. J Dent2016; 13(5): 349.. Dentin etching with phosphoric acid is performed to remove the smear layer 77. Hu X, Luong MN, Zhang H, Zhu H, Chan DC, Sadr A. Influence of phosphoric acid etching on the dentin bond durability of universal adhesives. J Adhes Sci Technol 2019; 33(21):2356-68.) and expose the collagen network that will be later infiltrated by the adhesive forming the hybrid layer 88. Vaidyanathan TK, Vaidyanathan J. Recent advances in the theory and mechanism of adhesive resin bonding to dentin: a critical review. J Biomed Mater Res B Appl Biomater2009; 88(2): 558-78.. However, phosphoric acid creates a delicate collagen network that is depleted of hydroxyapatite and that would collapse upon drying preventing the effective infiltration of the adhesive 99. Prati C, Chersoni S, Pashley DH. Effect of removal of surface collagen fibrils on resin-dentin bonding. Dent Mater1999; 15(5): 323-31.,1010. El Feninat F, Ellis TH, Sacher E, Stangel I. A tapping mode AFM study of collapse and denaturation in dentinal collagen. Dent Mater2001; 17(4): 284-8..
Recently, an adhesive categorized as “universal” or “multi-mode”, as it can be used in both etch-and-rinse and self-etch modes, has been introduced 1111. Munoz MA, Luque-Martinez I, Malaquias P, Hass V, Reis A, Campanha NH , et al. In vitro longevity of bonding properties of universal adhesives to dentin. Oper Dent2015; 40: 282-92.. Different monomers and primers such as silane and 10-methacryloyloxydecyldihydrogen phosphate (MDP) are incorporated in some universal adhesive systems to improve their bonding effectiveness to the tooth structure 1212. Yoshihara K, Nagaoka N, Sonoda A, Maruo Y, Makita Y, Okihara T, et al. Effectiveness and stability of silane coupling agent incorporated in ‘universal’adhesives. Dent Mater2016; 32(10): 1218-25.. The bond strength of universal adhesives was acceptable with different etching protocols 1313. Rosa WL, Piva E, Silva AF. Bond strength of universal adhesives: a systematic review and meta-analysis. J Dent2015; 43: 765-76.; however, there is still debate about the ideal mode of application of universal adhesives, whether etch-and-rinse or self-etch 1414. Ahmed AA, Hassan MM, Abdalla AI. Microshear bond strength of universal adhesives to dentin used in total-etch and self-etch modes. Tanta Dent J2018; 15(2):91-8..
Phytic acid (IP6) is an organic acid present in our daily diet including cereals, legumes, oilseeds and nuts 1515. Schlemmer U, Frolich W, Prieto RM, Grases F. Phytate in foods and significance for humans: food sources, intake, processing, bioavailability, protective role and analysis. Mol Nutr Food Res2009; 53: S330-75.. It is a highly negatively charged molecule making it an effective chelator for multivalent cations such as calcium (Ca+2) 1616. Torres J, Domínguez S, Cerdá MF, Obal G, Mederos A, Irvine RF, et al. Solution behaviour of myo-inositol hexakisphosphate in the presence of multivalent cations: prediction of a neutral pentamagnesium species under cytosolic/nuclear conditions. J Inorg Biochem 2005; 99: 828-40.. Although it is currently used for removal of smear layer in endodontics 1717. Nassar M, Hiraishi N, Tamura Y, Otsuki M, Aoki K, Tagami J. Phytic acid: An alternative root canal chelating agent. J Endod2015; 41(2): 242-7., a limited number of studies were concerned about its use in improvement of bond strength to coronal dentin.
Therefore, the aim of this study was to investigate the effect of different concentrations and application times of IP6 on µTBS and nanoleakage of universal adhesive to deep dentin in comparison to PA etching or using the universal adhesive in SE mode. The tested null hypothesis was that IP6 had no significant effect on µTBS and nanoleakage to deep dentin.
Materials and Methods
The materials used in this study are described in Box 1.
Selection of teeth
A total of 48 intact, non-carious, freshly permanent human molar teeth extracted from 20- to 40- years old individuals for periodontal reasons were used in this study for preparation of specimens for microtensile bond strength and nanoleakage tests. The sample size was calculated using G*Power software version 3.1.9.2 to detect the effect size of 0.25, a power of 85% and at a significant level of 5% (p<0.05) and a partial eta squared of 0.06. Teeth were selected according to the protocol approved by the Ethical Committee of the Faculty of Dentistry, Suez Canal University, Egypt (number 170/2019). Immediately after extraction, teeth were thoroughly washed under running water to remove blood and mucous, scaled to remove calculus and remnants of periodontal ligament tissue and polished with fine pumice and soft rubber cups at conventional speed. Teeth were examined for freedom of cracks using a magnifying lens (5x). All teeth exhibiting any signs of caries, microcracks or any other defective structure were discarded. The collected teeth were stored in normal saline plus 0.5% thymol until being used for no longer than 3 months 1818. Akman S, Akman M, Eskitascioglu G , Belli S. Influence of several fiber-reinforced composite restoration techniques on cusp movement and fracture strength of molar teeth. Int Endod J2011; 44:407-15..
Preparation of specimens
Teeth were fixed in acrylic resin blocks then mounted in an automated diamond saw (Isomet 4000, Buehler Ltd., Lake Bluff, USA), which was used for all sectioning procedures in this study. The occlusal enamel of all teeth was removed using diamond disc under water cooling to expose superficial dentin just beneath the central groove. Then, with size 2 (ADA size number) round carbide bur (DIA TESSIN, Switzerland), an indentation of 2mm depth in dentin was prepared. The depth of the indentation was guided using a rubber stopper mounted to the shaft of the round bur. Deep dentin was reached by removal of the occlusal surface with the same diamond disc under water cooling till the indentation disappears 1919. Juloski J, Carrabba M, Aragoneses JM, Forner L, Vichi A, Ferrari M. Microleakage of Class II restorations and microtensile bond strength to dentin of low-shrinkage composites. Am J Dent2013; 26(5):271-7.. The exposed dentin surfaces were then polished with wet 600-grit SiC abrasive paper for 60 seconds to create a standardized smear layer.
Microtensile bond strength (μTBS) testing
Forty specimens were used for the microtensile bond strength testing. Five specimens were used as a control group (n=5), where dentin surfaces were etched with 37% PA (Meta Biomed Co., Ltd., Cheongju-si, Chungbuk, Korea) for 15 sec then rinsed for 20 sec and blot-dried with a moist cotton pellet. Another five specimens didn’t receive any acid pre-treatment and the universal adhesive was applied in a self-etch mode (SE) (n=5). The remaining 30 specimens were divided according to concentration of IP6 solution (C) (Sigma-Aldrich Corp., St Louis, USA) into two main groups (n=15): C1 group, dentin surfaces were conditioned with 0.5% IP6 and C2 group, dentin surfaces were conditioned with 1% IP6. Specimens of IP6 groups were further subdivided into three subgroups (n=5) according to application time of IP6 solution (T) as follow: subgroup T1, 15 sec; subgroup T2, 30 sec and subgroup T3, 60 sec. IP6 solution was applied concerning its concentrations and application times using a plastic syringe and then dentin surfaces were rinsed for 10 sec and blot-dried.
The adhesive system (Single Bond Universal, 3M Deutschland GmbH) was applied to the exposed dentin surfaces according to manufacturer’s instructions then light-cured for 10 sec using a LED light curing unit (Elipar S10, 3MESPE, St Paul, MN, USA, light intensity 1200 mW/cm2). Nano-hybrid resin composite (Filtek™ Z250 XT, 3M ESPE) was then incrementally packed in two horizontal layers of 2 mm thickness to form resin composite blocks of 4 mm height using a teflon mold (8 x 8 x 4 mm). Each increment was light-cured for 10 sec according to manufacturer’s instructions at a right angle from the occlusal surface then all specimens were stored in distilled water at room temperature for 24 h.
Microtensile bond strength (μTBS) measurement
Specimens were mounted in a specially designed gripping attachment and serially sectioned in bucco-lingual direction to obtain slabs, then further sectioned to obtain (0.9 mm x 0.9 mm) resin composite/dentin beams 2020. Kong K, Hiraishi N, Nassar M, Otsuki M, Yiu CK, Tagami J. Effect of phytic acid etchant on resin-dentin bonding: Monomer penetration and stability of dentin collagen. J Prosthodont Res2016; 61(3):251-8.. The resultant beams were individually measured with a digital caliper and attached to geraldeli’s jig 2121. Perdigão J, Geraldeli S, Carmo AR, Dutra HR. In vivo influence of residual moisture on microtensile bond strengths on one-bottle adhesives. J Esthet Restor Dent 2002; 14:31-8. using cyanoacrylate glue (Zapit Dental Ventures of America Inc., Corona, CA, USA) 2222. Ahn J, Jung KH, Son S, Hur B, Kwon YH , Park JK. Effect of additional etching and ethanol-wet bonding on the dentin bond strength of one-step self-etch adhesives. Resto Dent & Endod2015; 40(1): 68-74. full stop. The jig was in turn mounted into a universal testing machine (Instron, MA, USA) with a load cell of 500 N at a cross-head speed of 0.5 mm/min and stressed under tension until failure. The μTBS was calculated in MegaPascal (MPa) by a software (Bluehill Lite software, England).
Nanoleakage evaluation
Eight specimens were used for nanoleakage evaluation, where one specimen was used for PA group (control) and one specimen was used for SE group. The remaining six specimens were divided according to concentration of IP6 into two main groups (n=3) and each group was further subdivided according to application time of IP6 (n=1) as mentioned before in μTBS testing. Specimens were stored in distilled water at room temperature for 24 h then were sectioned into slabs (approximately 1 mm-thick) by slow-speed diamond saw. One central slab were chosen from each tooth 2323. Makishi P, André CB, Ayres AP, Martins AL, Giannini M. Effect of storage time on bond strength and nanoleakage expression of universal adhesives bonded to dentin and etched enamel. Oper Dent2016; 41(3): 305-17. that were then coated with two layers of fast-drying nail varnish (Colorama, CEIL) away from the resin /dentin interface by 1 mm on each side 2424. Bakhsh TA, Al-Zayer M, Al-Sahwan N, Al-bahrani Z, Bakry AS, Jamleh AO, et al. Comparative SEM observation of silver-nitrate at resin-dentin interface: nanoleakage study. Oral Health Care2017; 2(2):1-5.. The prepared slabs were immersed in 50 % (W/V) ammonical silver nitrate (AgNO3) tracer solution for 24 h in black photo-film containers to ensure total darkness. Slabs were then rinsed with distilled water and immersed in a photo-developing solution (Kodak Professional D-76 developer, Kodak Rochester, NY) for 8 h under the effect of fluorescent light 2525. Hashimoto M, De Munck J, Ito S, Sano H, Kaga M, Oguchi H, et al. In vitro effect of nanoleakage expression on resin-dentin bond strengths analyzed by microtensile bond test, SEM/EDX and TEM. Biomater 2004; 25(25):5565-74.. Slabs were then wet-polished using 2000-grit SiC paper and diamond pastes (Buehler Ltd., Lake Bluff, IL, USA) 2626. Cardenas AF, Siqueira FS, Bandeca MC, Costa SO, Lemos MV, Feitora VP, et al. Impact of pH and application time of meta-phosphoric acid on resin-enamel and resin-dentin bonding. J Mech Behav Biomed Mater2018; 78:352-61., mounted on aluminum stubs and sputter-coated with gold (Edwards S150A, UK). Later on, slabs were observed using a field emission scanning electron microscope (FE-SEM) (QUANTA FEG 250) in backscattered electron mode with 20 kV and standardized 3000x magnification 2727. De-Paula DM, Lomonaco D, Ponte AM, Cordeiro KE, Moreira MM, Mazzetto SE, et al. Influence of collagen cross-linkers addition in phosphoric acid on dentin biomodification and bonding of an etch-and-rinse adhesive. Dent Mater2020; 36(1):e1-8.. Photomicrographs were obtained from each slab and silver nitrate uptake was evaluated using open-source Image J software (Image J, National Institute of Health, Bethesda, MD, USA).
Statistical analysis
The mean and standard deviation values were calculated for each group in each test. Data were explored for normality using Kolmogorov-Smirnov and Shapiro-Wilk tests, data showed parametric (normal) distribution. One-way ANOVA followed by Tukey post-hoc test was used to compare between more than two groups in non-related samples. Also, Two-way ANOVA was used to test the interaction between variables. The significance level was set at P ≤ 0.05. Statistical analysis was performed with IBM® SPSS® Statistics Version 20 for Windows.
Results
Microtensile bond strength results
The mean and standard deviation of μTBS values of the tested groups are presented in Table 1. The results showed that IP6 groups (0.5% and 1%) had significantly higher μTBS mean values compared to PA group (control) and SE group (p<0.001). There was no statistically significant difference between PA group and SE group (p>0.001). Regarding C1 group, the experimental subgroup C1T3 recorded the highest μTBS mean value followed by C1T2, while the least μTBS mean value was found in C1T1, with a statistically significant difference only between subgroups C1T1 and C1T3 (p<0.001). Regarding C2 group, the experimental subgroup C2T3 showed the highest μTBS mean value followed by C2T2, while the least μTBS mean value was found in C2T1. A statistically significant difference was found between C2T1 and each of C2T2 and C2T3 subgroups (p<0.001).
Nanoleakage results
FE-SEM photomicrographs showed different nanoleakage levels between groups. A distinctive silver-reticular pattern formation could be recognized along the hybrid layer of both PA and SE groups (Figure 1A and B) representing higher levels of nanoleakage. IP6 groups’ showed a decrease in nanoleakage levels along the hybrid layer that was represented by decrease in the thickness of the silver-reticular pattern as shown in the experimental subgroups C1T1, C1T2, C2T1 and C2T2 (Figure 2A, 2B, 3A & 3B). Increasing application time to 60 sec in both concentrations of IP6 resulted in distinct decrease in silver uptake that appears as spotted-pattern along the hybrid layer as shown in the experimental subgroups C1T3 and C2T3 (Figure 2C and 3C).
Representative FE-SEM photomicrographs of at (3000X) showing nanoleakage at the hybrid layer. (A) PA group (control), (B) SE group. The white arrows represent silver nitrate uptake, (c) composite, (a) adhesive and (d) dentin.
Representative FE-SEM photomicrographs at (3000X) showing nanoleakage at the hybrid layer. (A) Subgroup C1T1, (B) Subgroup C1T2 and (C) Subgroup C1T3. The white arrows represent silver nitrate uptake, (c) composite, (a) adhesive and (d) dentin.
Representative FE-SEM photomicrographs at (3000X) showing nanoleakage at the hybrid layer. (A) Subgroup C2T1, (B) Subgroup C2T2 and (C) Subgroup C2T3. The white arrows represent silver nitrate uptake, (c) composite, (a) adhesive and (d) dentin.
Discussion
Deep dentin is much more difficult to bond compared to superficial dentin due to its low contents of intertubular dentin as well as higher amount of water as reported in some studies 2828. Villela-Rosa AC, Gonc¸alves M, Orsi IA, Miani PK. Shear bond strength of self-etch and total-etch bonding systems at different dentin depths. Braz Oral Res2011; 25:109-15.,2929. Pegado RE, Do Amaral FL, Flório FM, Basting RT. Effect of different bonding strategies on adhesion to deep and superficial permanent dentin. Eur J Dent 2010; 4: 110-7.. Phosphoric acid has been widely used at concentrations of 35-37% for 15 sec for dentin etching 3030. Loguercio AD, Luque-Martinez I, Muñoz MA, Szesz AL, Cuadros-Sánchez J, Reis A. A comprehensive laboratory screening of three-step etch-and-rinse adhesives. Oper Dent2014; 39:652-62.. With these high concentrations, this acid creates a deep demineralized layer that may not be completely infiltrated by resin monomers 3131. Reis AF, Giannini M, Pereira PN. Long-term TEM analysis of the nanoleakage patterns in resin-dentin interfaces produced by different bonding strategies. Dent Mater2007; 23:1164-72.. This layer of demineralized dentin is left unprotected by resin forming a weak zone of the bonded interface 3232. Fuentes V, Ceballos L, Osorio R, Toledano M, Carvalho RM, Pashley DH. Tensile strength and microhardness of treated human dentin. Dent Mater2004; 20:522-9.. Adhesive systems named “universal” or “multimode” were introduced to promote adhesion to dentin 3333. Cardoso GC, Nakanishi L, Isolan CP, Jardim PD, Moraes RR. Bond stability of universal adhesives applied to dentin using etch-and-rinse or self-etch strategies. Braz Dent J2019; 30(5):467-75.. Single Bond Universal Adhesive was used in the current study which contains 10-MDP functional monomer which chemically interacts with hydroxyapatite forming a stable nanolayer that could constitute a strong phase at the adhesive interface 3434. Yoshida Y, Yoshihara K, Nagaoka N, Hayakawa S, Torii Y, Ogawa T, et al. Self-assembled nano-layering at the adhesive interface, J Dent Res2012; 91(4) 376-81.. Unfortunately, the lower calcium content which is needed for chemical bond with 10-MDP in addition to the increased dentin permeability in deep dentin may resulted in low bond strength values in deep dentin 3535. Gré CP, de Andrada MAC, Junior SM. Microtensile bond strength of a universal adhesive to deep dentin. Braz Dent Sci2016; 19(2):104-10.. Phytic acid is an organic acid found in cereals and legumes 1515. Schlemmer U, Frolich W, Prieto RM, Grases F. Phytate in foods and significance for humans: food sources, intake, processing, bioavailability, protective role and analysis. Mol Nutr Food Res2009; 53: S330-75. and it was proved to be an effective agent in removing smear layer in endodontic treatment 1717. Nassar M, Hiraishi N, Tamura Y, Otsuki M, Aoki K, Tagami J. Phytic acid: An alternative root canal chelating agent. J Endod2015; 41(2): 242-7.. It has a strong negative charge that can chelate positively charged multivalent cations of hydroxyapatite such as calcium (Ca+2) to form Ca-phytate salt which is characterized by very low solubility 3636. Veiga N, Torres J, Domínguez S, Mederos A, Irvine RF, Díaz A, et al. The behavior of myo-inositol hexakisphosphate in the presence of magnesium (II) and calcium (II): protein-free soluble InsP6 is limited to 49 µM under cytosolic/nuclear conditions. J Inorg Biochem 2006; 100:1800-10.,3737. Nassar M, Hiraishi N, Islam M, Romero MJ, Otsuki M, Tagami J. Effect of phytic acid as an endodontic chelator on resin adhesion to sodium hypochlorite-treated dentin. Restor Dent Endod2020; 45(4):e44..
The results of this study showed that application of IP6 at both concentrations (0.5 % and 1%) in groups C1 & C2 respectively recorded significantly higher μTBS mean values and less nanoleakage levels than PA group. This result was confirmed by its FE-SEM photomicrographs which showed a thinner reticular pattern of silver uptake along the hybrid layer of IP6 groups’ than that of PA group. This result could be attributed to that PA etching causes deep demineralization that jeopardizes complete infiltration of resin monomers, thereby resulting in the formation of a weaker and unprotected demineralized dentin zone at the base of the hybrid layer 3838. Hashimoto M, Ohno H, Kaga M, Sano H, Tay FR, Oguchi H, et al. Over-etching effects on micro-tensile bond strength and failure patterns for two dentin bonding systems. J Dent2002; 30(2-3):99-105.. This poor impregnation of resin could result in low bond strength 3939. Nakajima M, Okuda M, Pereira PN, Tagami J, Pashley DH. Dimensional changes and ultimate tensile strengths of wet decalcified dentin applied with one-bottle adhesives. Dent Mater2002; 18: 603-8..
The results also revealed that IP6 groups’ recorded significantly higher μTBS mean values than SE group. In consistence with this result, FE-SEM photomicrographs showed a thicker silver-reticular pattern of nanoleakage along the hybrid layer of SE group in comparison to IP6 groups’. This result could be attributed to the ultra-mild acidity of Single Bond Universal Adhesive (pH 2.7) which resulted in incomplete penetration of acidic monomers into the smear layer and its partial dissolution and consequent minimal penetration into dentin beneath the smear layer 4040. Carvalho RM, Chersoni S, Frankenberger R, Pashley DH, Prati C,Tay FR. A challenge to the conventional wisdom that simultaneous etching and resin infiltration always occurs in self-etch adhesives. Biomater 2005; 26(9):1035-42.. On the other hand, IP6 is more acidic (pH ≥ 1), so it has higher ability to remove the smear layer with a conditioning effect on the underlying dentin; this may have allowed better penetration of resin monomers into the demineralized dentin 2020. Kong K, Hiraishi N, Nassar M, Otsuki M, Yiu CK, Tagami J. Effect of phytic acid etchant on resin-dentin bonding: Monomer penetration and stability of dentin collagen. J Prosthodont Res2016; 61(3):251-8.. IP6 also may function as a natural crosslinker to collagen fibrils of the demineralized dentin, making them more stable and less susceptible to collapse, resulting in better preservation of the interfibrillar spaces to enable better impregnation of monomers 4141. Nassar M, Hiraishi N, Islam MS, Aizawa M, Tamura Y, Otsuki M, Kasugai S, Ohya K, Tagami J. Effect of phytic acid used as etchant on bond strength, smear layer, and pulpal cells. Eur J Oral Sci 2013; 121(5):482-7.,4242. Kong K, Islam MS, Nassar M, Hiraishi N, Otsuki M, Yiu CK, et al. Effect of phytic acid etchant on the structural stability of demineralized dentine and dentine bonding. J Mech Behav Biomed Mater2015; 48:145-52.. The cross-linking effect of IP6 to collagen may be related to hydrogen bond that occurs between its hydroxyl groups and the amine groups of the side chain amino acid in collagen molecule 4343. Cristina MPV, Thaiane RA, Rasika P, James BM, Jose GN, Shao NC, et al. Galloyl moieties enhance the dentin biomodification potential of plant-derived catechins. Acta Biomaterialia2014; 10:3288-94.. Additionally, IP6 can bind to protein and calcium to form a ternary complex (Protein-Ca-Phytate) which has a good chemical bond 4444. Cheryan M. Phytic acid interactions in food systems. Crit Rev Food Sci Nutr 1980; 13:297-335..
Regarding the effect of IP6 concentration, the results showed that C1group (0.5% IP6) recorded higher μTBS mean values and less nanoleakage levels than C2 group (1% IP6) group. This may be explained on the basis of that dentin conditioning with higher concentration of acids can result in excessive intertubular dentin demineralization and collagen collapse with suspected decrease in μTBS values 4545. Gateva N, Gusyiska A, Stanimirov P, Kabaktchieva R, Raichev I. Effect of etching time and acid concentration on micromorphological changes in dentin of both dentitions. J IMAB2016; 22(2):1099-110..
Considering the effect of application time of IP6, the results revealed that increasing application time of IP6 had a positive effect on μTBS mean values to deep dentin. The results showed that the application of IP6 for 60 sec recorded significantly higher μTBS mean value than 30 sec and 15 sec respectively. Nanoleakage results also were in accordance with μTBS values, where increasing the conditioning time showed a distinct decrease in silver uptake along the hybrid layer from reticular-pattern to spotted-pattern as shown in FE-SEM photomicrographs. This result could be attributed to the fact that longer application time promote more dissolution of the smear layer on the dentin surface for better resin monomer diffusion, allowing improved mechanical interlocking and consequently higher resin-dentin µTBS 4646. Botelho MP, Isolan CP, Schwantz JK, Lopes MB, Moraes RR. Rubbing time and bonding performance of one-step adhesives to primary enamel and dentin. J Appl Oral Sci 2017; 25: 523-32..
In the present study, the use of IP6 to condition deep dentin surface significantly improved µTBS and nanoleakage of universal adhesive in comparison to phosphoric acid etching or using the universal adhesive in a self-etch mode. Thus, the null hypothesis was rejected.
Recommendations
Further in vitro studies are needed to assess the effect of aging on microtensile bond strength and interfacial integrity of universal adhesive to deep dentin after conditioning with phytic acid.
Further in vivo studies are needed to assess the effect of phytic acid on microtensile bond strength and interfacial integrity of universal adhesive to deep dentin.
It is recommended to supply phytic acid in gel form for better manipulation than liquid form.
Conclusions
Under the limitations of this in vitro study, the following could be concluded:
Conditioning of deep dentin with phytic acid (either 0.5% or 1%) enhance microtensile bond strength and interfacial integrity of universal adhesive to deep dentin in comparison to phosphoric acid etching or using the universal adhesive in a self-etch mode.
Increasing application time of phytic acid improves microtensile bond strength as well as interfacial integrity of universal adhesive to deep dentin.
References
-
1Sharafeddin F, Nouri H, Koohpeima F. The effect of temperature on shear bond strength of clearfil SE bond and adper single bond adhesive systems to dentin. J Dent Shiraz Univ Med Sci 2015; 16(1):10-6.
-
2Featherstone JD, Lussi A. Understanding the chemistry of dental erosion. Monogr. Oral Sci2006; 20: 66-76.
-
3Pashley DH, Tay FR, Breschi L, Tjäderhane L, Carvalho RM, Carrilho M, et al. State of the art etch-and-rinse adhesives. Dent Mater2011; 27(1): 1-16.
-
4Akbarian S, Sharafeddin F, Akbarian G. Evaluation of the influence of three different temperatures on microleakage of two self-etch and one total-etch adhesives. J Contemp Dent Pract2015; 16(3): 178-82.
-
5Kinney JH, Balooch M, Marshall SJ, Marshall GW Jr, Weihs TP. Atomic force microscope measurements of the hardness and elasticity of peritubular and intertubular human dentin. J Biomech Eng1996; 118: 133-35.
-
6Mosharrafian S, Afshar H, Farbod M , Baniameri Z. Effect of etching time and preparation on push-out bond strength of composite to intracanal dentin of primary anterior teeth. J Dent2016; 13(5): 349.
-
7Hu X, Luong MN, Zhang H, Zhu H, Chan DC, Sadr A. Influence of phosphoric acid etching on the dentin bond durability of universal adhesives. J Adhes Sci Technol 2019; 33(21):2356-68.
-
8Vaidyanathan TK, Vaidyanathan J. Recent advances in the theory and mechanism of adhesive resin bonding to dentin: a critical review. J Biomed Mater Res B Appl Biomater2009; 88(2): 558-78.
-
9Prati C, Chersoni S, Pashley DH. Effect of removal of surface collagen fibrils on resin-dentin bonding. Dent Mater1999; 15(5): 323-31.
-
10El Feninat F, Ellis TH, Sacher E, Stangel I. A tapping mode AFM study of collapse and denaturation in dentinal collagen. Dent Mater2001; 17(4): 284-8.
-
11Munoz MA, Luque-Martinez I, Malaquias P, Hass V, Reis A, Campanha NH , et al. In vitro longevity of bonding properties of universal adhesives to dentin. Oper Dent2015; 40: 282-92.
-
12Yoshihara K, Nagaoka N, Sonoda A, Maruo Y, Makita Y, Okihara T, et al. Effectiveness and stability of silane coupling agent incorporated in ‘universal’adhesives. Dent Mater2016; 32(10): 1218-25.
-
13Rosa WL, Piva E, Silva AF. Bond strength of universal adhesives: a systematic review and meta-analysis. J Dent2015; 43: 765-76.
-
14Ahmed AA, Hassan MM, Abdalla AI. Microshear bond strength of universal adhesives to dentin used in total-etch and self-etch modes. Tanta Dent J2018; 15(2):91-8.
-
15Schlemmer U, Frolich W, Prieto RM, Grases F. Phytate in foods and significance for humans: food sources, intake, processing, bioavailability, protective role and analysis. Mol Nutr Food Res2009; 53: S330-75.
-
16Torres J, Domínguez S, Cerdá MF, Obal G, Mederos A, Irvine RF, et al. Solution behaviour of myo-inositol hexakisphosphate in the presence of multivalent cations: prediction of a neutral pentamagnesium species under cytosolic/nuclear conditions. J Inorg Biochem 2005; 99: 828-40.
-
17Nassar M, Hiraishi N, Tamura Y, Otsuki M, Aoki K, Tagami J. Phytic acid: An alternative root canal chelating agent. J Endod2015; 41(2): 242-7.
-
18Akman S, Akman M, Eskitascioglu G , Belli S. Influence of several fiber-reinforced composite restoration techniques on cusp movement and fracture strength of molar teeth. Int Endod J2011; 44:407-15.
-
19Juloski J, Carrabba M, Aragoneses JM, Forner L, Vichi A, Ferrari M. Microleakage of Class II restorations and microtensile bond strength to dentin of low-shrinkage composites. Am J Dent2013; 26(5):271-7.
-
20Kong K, Hiraishi N, Nassar M, Otsuki M, Yiu CK, Tagami J. Effect of phytic acid etchant on resin-dentin bonding: Monomer penetration and stability of dentin collagen. J Prosthodont Res2016; 61(3):251-8.
-
21Perdigão J, Geraldeli S, Carmo AR, Dutra HR. In vivo influence of residual moisture on microtensile bond strengths on one-bottle adhesives. J Esthet Restor Dent 2002; 14:31-8.
-
22Ahn J, Jung KH, Son S, Hur B, Kwon YH , Park JK. Effect of additional etching and ethanol-wet bonding on the dentin bond strength of one-step self-etch adhesives. Resto Dent & Endod2015; 40(1): 68-74.
-
23Makishi P, André CB, Ayres AP, Martins AL, Giannini M. Effect of storage time on bond strength and nanoleakage expression of universal adhesives bonded to dentin and etched enamel. Oper Dent2016; 41(3): 305-17.
-
24Bakhsh TA, Al-Zayer M, Al-Sahwan N, Al-bahrani Z, Bakry AS, Jamleh AO, et al. Comparative SEM observation of silver-nitrate at resin-dentin interface: nanoleakage study. Oral Health Care2017; 2(2):1-5.
-
25Hashimoto M, De Munck J, Ito S, Sano H, Kaga M, Oguchi H, et al. In vitro effect of nanoleakage expression on resin-dentin bond strengths analyzed by microtensile bond test, SEM/EDX and TEM. Biomater 2004; 25(25):5565-74.
-
26Cardenas AF, Siqueira FS, Bandeca MC, Costa SO, Lemos MV, Feitora VP, et al. Impact of pH and application time of meta-phosphoric acid on resin-enamel and resin-dentin bonding. J Mech Behav Biomed Mater2018; 78:352-61.
-
27De-Paula DM, Lomonaco D, Ponte AM, Cordeiro KE, Moreira MM, Mazzetto SE, et al. Influence of collagen cross-linkers addition in phosphoric acid on dentin biomodification and bonding of an etch-and-rinse adhesive. Dent Mater2020; 36(1):e1-8.
-
28Villela-Rosa AC, Gonc¸alves M, Orsi IA, Miani PK. Shear bond strength of self-etch and total-etch bonding systems at different dentin depths. Braz Oral Res2011; 25:109-15.
-
29Pegado RE, Do Amaral FL, Flório FM, Basting RT. Effect of different bonding strategies on adhesion to deep and superficial permanent dentin. Eur J Dent 2010; 4: 110-7.
-
30Loguercio AD, Luque-Martinez I, Muñoz MA, Szesz AL, Cuadros-Sánchez J, Reis A. A comprehensive laboratory screening of three-step etch-and-rinse adhesives. Oper Dent2014; 39:652-62.
-
31Reis AF, Giannini M, Pereira PN. Long-term TEM analysis of the nanoleakage patterns in resin-dentin interfaces produced by different bonding strategies. Dent Mater2007; 23:1164-72.
-
32Fuentes V, Ceballos L, Osorio R, Toledano M, Carvalho RM, Pashley DH. Tensile strength and microhardness of treated human dentin. Dent Mater2004; 20:522-9.
-
33Cardoso GC, Nakanishi L, Isolan CP, Jardim PD, Moraes RR. Bond stability of universal adhesives applied to dentin using etch-and-rinse or self-etch strategies. Braz Dent J2019; 30(5):467-75.
-
34Yoshida Y, Yoshihara K, Nagaoka N, Hayakawa S, Torii Y, Ogawa T, et al. Self-assembled nano-layering at the adhesive interface, J Dent Res2012; 91(4) 376-81.
-
35Gré CP, de Andrada MAC, Junior SM. Microtensile bond strength of a universal adhesive to deep dentin. Braz Dent Sci2016; 19(2):104-10.
-
36Veiga N, Torres J, Domínguez S, Mederos A, Irvine RF, Díaz A, et al. The behavior of myo-inositol hexakisphosphate in the presence of magnesium (II) and calcium (II): protein-free soluble InsP6 is limited to 49 µM under cytosolic/nuclear conditions. J Inorg Biochem 2006; 100:1800-10.
-
37Nassar M, Hiraishi N, Islam M, Romero MJ, Otsuki M, Tagami J. Effect of phytic acid as an endodontic chelator on resin adhesion to sodium hypochlorite-treated dentin. Restor Dent Endod2020; 45(4):e44.
-
38Hashimoto M, Ohno H, Kaga M, Sano H, Tay FR, Oguchi H, et al. Over-etching effects on micro-tensile bond strength and failure patterns for two dentin bonding systems. J Dent2002; 30(2-3):99-105.
-
39Nakajima M, Okuda M, Pereira PN, Tagami J, Pashley DH. Dimensional changes and ultimate tensile strengths of wet decalcified dentin applied with one-bottle adhesives. Dent Mater2002; 18: 603-8.
-
40Carvalho RM, Chersoni S, Frankenberger R, Pashley DH, Prati C,Tay FR. A challenge to the conventional wisdom that simultaneous etching and resin infiltration always occurs in self-etch adhesives. Biomater 2005; 26(9):1035-42.
-
41Nassar M, Hiraishi N, Islam MS, Aizawa M, Tamura Y, Otsuki M, Kasugai S, Ohya K, Tagami J. Effect of phytic acid used as etchant on bond strength, smear layer, and pulpal cells. Eur J Oral Sci 2013; 121(5):482-7.
-
42Kong K, Islam MS, Nassar M, Hiraishi N, Otsuki M, Yiu CK, et al. Effect of phytic acid etchant on the structural stability of demineralized dentine and dentine bonding. J Mech Behav Biomed Mater2015; 48:145-52.
-
43Cristina MPV, Thaiane RA, Rasika P, James BM, Jose GN, Shao NC, et al. Galloyl moieties enhance the dentin biomodification potential of plant-derived catechins. Acta Biomaterialia2014; 10:3288-94.
-
44Cheryan M. Phytic acid interactions in food systems. Crit Rev Food Sci Nutr 1980; 13:297-335.
-
45Gateva N, Gusyiska A, Stanimirov P, Kabaktchieva R, Raichev I. Effect of etching time and acid concentration on micromorphological changes in dentin of both dentitions. J IMAB2016; 22(2):1099-110.
-
46Botelho MP, Isolan CP, Schwantz JK, Lopes MB, Moraes RR. Rubbing time and bonding performance of one-step adhesives to primary enamel and dentin. J Appl Oral Sci 2017; 25: 523-32.
Publication Dates
-
Publication in this collection
21 Oct 2022 -
Date of issue
Sep-Oct 2022
History
-
Received
11 Aug 2021 -
Accepted
13 July 2022